SINOCLEAN logo Request a quote

Manufacturing · Microfiber factory

Inside SINOCLEAN's microfiber cloth factory in China: every stage, photographed

SINOCLEAN is a microfiber cloth manufacturer in China, and most suppliers in this trade describe microfiber as a material. It is a route — and the difference between two “microfiber” cloths is usually a stage one factory runs and the other does not. This page follows the cloth through our own works in the order it actually moves, from the texturing machines that make the yarn to the carton in the finished-goods store, including the wholesale and private-label options each stage allows.

Photographed inside our texturing, knitting, dyeing and converting works · 2026-11-22 ·

The short answer. Texturing → warping → knitting → greige inspection → batch sewing → desizing → alkali weight reduction (splitting) → dyeing → centrifugal extraction → opening → stenter setting. The dyed roll then returns to the converting building: head cut and slit, first overlock on the strip, automatic overlock to piece, manual overlock for custom shapes, template sewing, ultrasonic sealing or hot cutting, perforating, packing, finished goods. Splitting is the stage that makes the cloth microfiber; every other stage either protects what it produced or turns it into a product.

Microfiber cloth is a knitted or woven fabric made from filaments finer than one decitex. It is produced by knitting a bicomponent yarn and then splitting that yarn in an alkali bath, so each thick filament divides into many microfilaments. The cloth is then dyed, set, cut and edge-sealed. That definition matters commercially: a cloth made from fine-denier polyester without splitting is not microfiber, however soft it feels.

At a glance

Company
JINHUA SINOCLEAN CO., LTD, founded 2014
What we are
Microfiber cloth manufacturer and exporter, Jinhua, Zhejiang, China
In-house steps
Texturing, warping, warp knitting, alkali weight reduction, dyeing, converting
MOQ
3,000 pcs per item and colour; Pantone-matched colours up to 5,000
Samples
Stock 5–7 days; custom 10–15 days
Production
25–35 days after deposit
Ports
Ningbo / Shanghai · FOB, CIF, EXW, DDP
Inspection
AQL 2.5 pre-shipment; third-party inspection welcome

Stage 01 of 22

Draw texturing#

Draw texturing (DTY) — composite yarn, textured in-house

Draw texturing is the process that turns partially oriented yarn into a drawn, bulky yarn with controlled elongation.

Our route starts one step earlier than most factories describe theirs. The bicomponent yarn arrives as POY — partially oriented — and is drawn and textured on our own machines: heated, false-twisted, cooled and wound into a package with controlled bulk and elongation.

This matters to a buyer for two reasons. Bulk decides how the knitted loop fills out, so it sets the hand and the thickness of the finished cloth before any cloth exists. Elongation decides how the yarn behaves on the warper, where several thousand ends are pulled at once.

What we control, and what goes wrong

Because the yarn is textured in-house, a change in bulk or in oil finish does not depend on a supplier's delivery. That is the first of the three places where a microfiber factory is either the producer or the buyer — the other two are splitting and dyeing.

Equipment
Draw-texturing machines
We control
Draw ratio, texturing temperature, spindle speed, oil finish, package weight
If it drifts
Barré — bands across the finished cloth that no dye bath can correct

What you can specify Yarn spec and count; whether the yarn is textured in-house or bought in.

All 22 stages in one table

Texturing hall: yarn packages staged before the texturing positions.
Texturing hall: yarn packages staged before the texturing positions.
Creel banks feeding the texturing line, one package per position.
Creel banks feeding the texturing line, one package per position.
Package shelves in the same hall — supply staged by lot.
Package shelves in the same hall — supply staged by lot.
Composite yarn packages, close up: this is the yarn that becomes the cloth.
Composite yarn packages, close up: this is the yarn that becomes the cloth.
Aisle between creel banks. Several thousand packages run at once.
Aisle between creel banks. Several thousand packages run at once.

Stage 02 of 22

Warping#

Warping — creel to beam

Warping is the stage that gathers every warp end onto one beam at matched tension.

Warp knitting consumes yarn lengthwise, so the first thing that has to exist is a beam: several thousand ends wound side by side at the same tension, one package per end.

This is the stage where a single mistake cannot be hidden. One wrong end runs as a visible line down the entire beam. One slack end becomes a stripe after dyeing, because it takes up dye differently from its neighbours. A beam wound unevenly produces cloth that looks correct on the roll and curls at the edge once it has been through the dyebath.

What we control, and what goes wrong

The beam also fixes the fabric's width, and more subtly its flatness. Buyers who complain about edge curl are usually looking at a warping problem three stages upstream.

Equipment
Warping creel and beaming machine
We control
End tension across the full sheet, beam build density, broken-end stop
If it drifts
Width variation between rolls, edge curl, and a beam that has to be cut off and rewound

What you can specify Beam width and ends per beam - these fix the maximum fabric width.

All 22 stages in one table

Warping line: the beam being built at the head of the creel.
Warping line: the beam being built at the head of the creel.
Creel wall — each package carries one warp end.
Creel wall — each package carries one warp end.
Warp beam and creel in the same frame; the sheet runs from creel to beam.
Warp beam and creel in the same frame; the sheet runs from creel to beam.
Beam storage beside the line, ready to be mounted on the knitting machine.
Beam storage beside the line, ready to be mounted on the knitting machine.
Beaming head: the warp sheet - one end per package - is wound onto the beam under tension.
Beaming head: the warp sheet - one end per package - is wound onto the beam under tension.

Stage 03 of 22

Knitting#

Warp knitting — tricot construction

Warp knitting is a loop-forming process in which the yarn systems run along the fabric rather than across it.

The beam is mounted and the cloth is knitted. Warp knitting builds loops from yarn systems running along the fabric, which is why warp-knitted microfiber holds its shape and does not distort when wrung — the usual choice for cleaning, glass and car cloths.

The surface names a catalogue sells are not separate materials. Grid, pearl, waffle and fishscale are lapping patterns set on the same machine; the yarn and the pattern change, the process does not. Coral fleece and terry come off circular machines instead, forming courses across the fabric for a softer, stretchier hand.

What we control, and what goes wrong

What leaves this stage is greige: undyed, unfinished, still carrying knitting oil. Everything after it changes the cloth's colour and surface, but nothing after it can change the structure that was knitted here.

Equipment
Warp-knitting (tricot) and circular machines
We control
Needle gauge, working width, lapping pattern, yarn tension
Output
Greige at the knitted width and GSM, wound onto a batch beam
If it drifts
A GSM that repeats on the sample and not on bulk — the commonest source of “the second shipment feels different”

What you can specify GSM, working width, needle gauge and the lapping pattern (grid, pearl, waffle, fishscale).

All 22 stages in one table

Warp sheet entering the needle bed: thousands of parallel ends.
Warp sheet entering the needle bed: thousands of parallel ends.
Cloth leaving the needle bed and running to the batch beam.
Cloth leaving the needle bed and running to the batch beam.
Warp-knitting machine in operation, greige on the beam.
Warp-knitting machine in operation, greige on the beam.
Machine row: the same pattern is set on each machine, not bought as a different material.
Machine row: the same pattern is set on each machine, not bought as a different material.

Stage 04 of 22

Greige inspection#

Greige inspection — grading before wet processing

Greige inspection is the grading of undyed cloth against width, GSM and defect standards before wet processing.

Rolls are checked for width, GSM and surface defects, then separated by lot and graded. The point is timing: a fault found now can be reassigned to a shorter cut or a lower grade, while a fault found after dyeing carries the cost of the dye, the alkali and the energy already spent on it.

The record produced here is what makes a shade complaint traceable later. Roll number, lot, metres and defect map travel with the cloth into the dyehouse, so a finished carton can be traced back to the batch it came from.

What we control, and what goes wrong

We control
Width, GSM and defect map per roll; rolls graded and lot-tagged
If it drifts
Mixed widths inside one carton, and cloth cut to a size that no longer matches the printed pack

What you can specify Accepted defect level, and whether grading is per roll or per lot.

All 22 stages in one table

Inspection and grading area, rolls staged by lot.
Inspection and grading area, rolls staged by lot.
Cloth spread for grading before it is released to the dyehouse.
Cloth spread for grading before it is released to the dyehouse.

Stage 05 of 22

Greige store#

Greige store — waiting for the dyehouse

The greige store is the buffer between knitting and dyeing, where rolls are held by lot.

Greige is stored rather than pushed straight into the dyehouse, because dyeing is scheduled by colour and machine load, not by knitting order. Holding the rolls by lot is what keeps a dye batch consistent when two knitting lots are waiting.

This is the handover point between the two halves of the factory. The lot tag applied here is the same identifier that later appears on the dyed roll in the converting store.

What we control, and what goes wrong

We control
Lot identification, roll count and metres, storage condition, release by lot
If it drifts
Two knitting lots mixed into one dye batch, with no way back to the source

What you can specify Nothing visible - but the lot discipline behind it decides shade traceability later.

All 22 stages in one table

Greige rolls stored by lot, waiting for a dye slot.
Greige rolls stored by lot, waiting for a dye slot.
B

Wet processing

The greige is joined, desized and split, dyed, dewatered, opened and set. This is where the cloth becomes microfiber.

Stage 06 of 22

Batch sewing#

Batch sewing — joining roll to roll

Batch sewing is the joining of two rolls end to end so the cloth runs continuously through wet processing.

A dye vessel and a stenter both want continuous cloth. Batch sewing joins the rolls so the line does not have to be stopped and rethreaded between them.

The join has to survive the dyebath and the stenter without marking the cloth either side of it. It is also why the first metres of a finished roll are cut away at head cutting: the join and the gripped head are both removed before anything is sealed or packed.

What we control, and what goes wrong

Equipment
Batch sewing machine
We control
Join strength, seam type, stitch depth clear of the usable surface
If it drifts
A join that pulls apart mid-batch, or a seam mark that shows as a band in the finished roll

What you can specify That the join is removed before packing; it is, at head cutting.

All 22 stages in one table

Cloth truck at the head of the dyehouse line, where rolls are joined.
Cloth truck at the head of the dyehouse line, where rolls are joined.

Stage 07 of 22

Desizing and scouring#

Desizing and scouring — same line as splitting

Desizing is open-width washing that removes knitting oil and sizing before the alkali is applied.

Knitting leaves oil, sizing and wax on the yarn. None of it is visible, and all of it matters: a film of knitting oil stops caustic soda from wetting the fibre evenly, so the reduction in the next stage lands unevenly and the cloth ends up half-split.

On our line desizing and alkali weight reduction are two stages of one continuous open-width range, which is why the two photographs in this section come from the same equipment. Running them as one pass means the cloth never dries between washing and reduction.

What we control, and what goes wrong

This is the stage most published descriptions of microfiber skip. It produces no visible change and it is the difference between a uniform split and a patchy one that only shows up two stages later as a shade complaint.

Equipment
Open-width wash range, continuous into the reduction bath
We control
Residual oil and sizing, water temperature, wettability, running width
If it drifts
Uneven splitting, then patchy dye uptake, then a shade complaint that appears two stages later than its cause

What you can specify Wash temperature and residual-oil target, if you specify them at all.

All 22 stages in one table

The open-width range: washing runs straight into the alkali bath on the same line.
The open-width range: washing runs straight into the alkali bath on the same line.

The defining stage

Stage 08 of 22

Alkali weight reduction (splitting)#

Alkali weight reduction — the step that creates microfiber

Alkali weight reduction - splitting - is the caustic treatment that divides each composite filament into microfilaments.

In sea-island fibre, caustic soda dissolves the Co-PET sea and leaves the polyester islands standing free. In segmented-pie fibre it separates the polyester and polyamide wedges. One thick filament becomes many, and the cloth that leaves this bath is finer than anything the knitting machine could have handled.

Three variables set the result: sodium hydroxide concentration, temperature and dwell time. Together they fix the weight loss, and the weight loss fixes how fine the filaments end up.

What we control, and what goes wrong

Under-reduced cloth still feels soft, because the filaments at the surface are fine while the bundle underneath is still glued together — and it wipes like ordinary polyester. Over-reduced cloth loses strength and develops a limp, chalky hand that no stenter can correct. This is the one stage where a mistake cannot be recovered later, which is why it is the stage we measure rather than judge by feel.

Equipment
Alkali weight-reduction line
We control
NaOH concentration, temperature, dwell time, weight loss, resulting filament fineness
If it drifts
Under-reduced: soft but not absorbent, linting, streaks on glass. Over-reduced: weak cloth, chalky hand, seam failure at sewing

What you can specify Weight loss and resulting filament fineness - the two numbers that define the cloth.

All 22 stages in one table

The reduction line. Cloth runs enclosed through the alkali and the wash compartments.
The reduction line. Cloth runs enclosed through the alkali and the wash compartments.

Stage 09 of 22

Dyeing#

Overflow dyeing — rope form

Overflow dyeing is a batch process in which cloth circulates as a rope through the dye liquor under temperature and pressure.

Fabric is dyed only after splitting, because dye has to reach filaments that are already open. Dyeing first and splitting afterwards gives a mottled result that no re-dye fully corrects.

Polyester needs disperse dye at high temperature under pressure; the polyamide component takes acid dye, and some works run both in one alkaline bath to save a cycle. Because the two polymers dye by different mechanisms, the ratio fixed at the yarn stage resurfaces here as depth and tone — an 80/20 cloth and a 90/20 cloth of the same nominal colour do not look identical side by side.

What we control, and what goes wrong

The number painted on the truck is the lot. Colour, recipe and batch size are all tied to it, and that same number follows the roll back to the converting building.

Equipment
Overflow dyeing machines
We control
Recipe, temperature curve, batch size, liquor ratio, lot number per batch
If it drifts
Uneven penetration that looks acceptable dry and goes patchy after the customer's first wash

What you can specify Colour standard, metamerism tolerance, and whether the lot number appears on the roll label.

All 22 stages in one table

Batch trucks at the dyehouse. The painted number is the lot.
Batch trucks at the dyehouse. The painted number is the lot.
Rope form leaving the dye vessel — the cloth is a twisted rope at this point, not a flat sheet.
Rope form leaving the dye vessel — the cloth is a twisted rope at this point, not a flat sheet.

Stage 10 of 22

Centrifugal extraction#

Centrifugal extraction — water removal

Centrifugal extraction is the dewatering step that removes most of the liquor before the cloth is opened.

Centrifugal extraction takes the bulk of the water out in seconds per batch, instead of letting the cloth drain. What matters downstream is the residual moisture, not the speed: cloth that reaches the stenter too wet carries water marks that the heat then sets permanently into the fabric.

Each truck of cloth goes into the extractor as one lot, so the batch identity survives the step.

What we control, and what goes wrong

Equipment
Centrifugal hydro-extractors
We control
Residual moisture, batch separation, damage at the basket wall
If it drifts
Water marks set by the stenter, and rope creases that cannot be removed afterwards

What you can specify Residual moisture before the stenter.

All 22 stages in one table

Centrifugal extractors, with dyed cloth waiting in lot-numbered trucks.
Centrifugal extractors, with dyed cloth waiting in lot-numbered trucks.

Stage 11 of 22

Opening#

Opening — rope back to flat width

Opening is the step that converts rope-form cloth back to flat width before drying and setting.

Cloth leaves the dye vessel as a twisted rope and has to be got back to flat width before anything else can be done to it. The rope is opened over a spreader, with moisture controlled on the way out.

This is also the first point since knitting where the full width can be measured, so width defects introduced upstream become visible here — and it is the last chance to remove a crease before the stenter fixes it.

What we control, and what goes wrong

Equipment
Fabric opener / detwister
We control
Opened width, creases, rope marks, running tension
If it drifts
Creases set by the stenter and impossible to remove afterwards; width short of specification

What you can specify Finished width tolerance, and whether rope marks are acceptable on the face.

All 22 stages in one table

Opening: cloth coming out of rope form over the spreader, on its way to the stenter.
Opening: cloth coming out of rope form over the spreader, on its way to the stenter.

Stage 12 of 22

Drying, heat-setting and batching#

Stenter and heat-setting — then batching

Heat-setting is the controlled application of width, tension and temperature that fixes GSM, width and residual shrinkage.

The stenter is where a length of fabric becomes a specified product: pulled to its finished width, held under tension through a heated chamber, and delivered with shrinkage, width and GSM locked.

Drying and heat-setting are not the same step. A line that only dries produces cloth that measures correctly in the warehouse and shrinks inside the customer's pack — the difference between the two is temperature, tension and the overfeed setting.

What we control, and what goes wrong

Overfeed controls how much length is allowed to relax into the frame, which is why the same greige can leave the stenter at two different weights, and why a GSM quoted without an overfeed figure is only half a specification. At the end of the line the cloth is batched into a roll and labelled with its lot before it goes back to the converting building.

Equipment
Stenter (tenter frame) with batching head
We control
Finished width, GSM after setting, residual shrinkage, overfeed, batch label
If it drifts
Cloth that measures correctly in the warehouse and shrinks after the first wash

What you can specify Width, GSM, overfeed and residual shrinkage - a GSM quoted without overfeed is half a spec.

All 22 stages in one table

Stenter line: the heated chamber where width and shrinkage are set.
Stenter line: the heated chamber where width and shrinkage are set.
Infeed: wet cloth entering the frame.
Infeed: wet cloth entering the frame.
Fabric web over the rollers, under tension, before batching.
Fabric web over the rollers, under tension, before batching.
Batched roll leaving the line, labelled for the converting store.
Batched roll leaving the line, labelled for the converting store.
C

Converting

The dyed roll comes back to this building: cut, slit, overlocked, template-sewn, sealed, perforated, packed and stored.

Stage 13 of 22

Back to the converting building#

Return and ground-floor store

The converting store is where dyed rolls are booked in by lot and held between dyeing and cutting.

The cloth does not leave the factory at this point — it returns to the converting building, the same building where it was knitted. The dyed rolls are booked into the ground-floor store by lot and wait for the converting floor to call them.

This return trip is the clearest sign of a factory that owns both halves of the process: knitting and dyeing on one side, converting on the other, with the same lot number carried across. A trader describing someone else's process cannot show it.

What we control, and what goes wrong

We control
Lot identification, metres per roll, storage condition, release to converting by lot
If it drifts
Two dye batches mixed inside one shipment — a shade complaint on an order that tested fine

What you can specify Lot traceability from carton back to dye batch.

All 22 stages in one table

Ground-floor store: dyed rolls shelved by lot, waiting for the converting floor.
Ground-floor store: dyed rolls shelved by lot, waiting for the converting floor.

Stage 14 of 22

Head cutting and slitting#

Head cutting and slitting

Head cutting is the removal of the damaged leading metres; slitting is the division of the roll to finished width.

Head cutting removes the leading metres that were gripped, stitched or clamped in the dye machine, including the join made at batch sewing. Nothing that carries the mark of the dyehouse goes into a finished cloth.

Slitting then divides the roll to the width the product needs: a single dyed roll may become several narrower strips, each of which will be edge-closed and then cut to piece length.

What we control, and what goes wrong

The position of this cut decides where the sealed or overlocked edge will sit. Cut it wide and the finished cloth is oversized; cut it narrow and the edge lands inside the wiping surface.

Equipment
Slitting machine with edge trim
We control
Finished width, slit count per roll, head waste removed, edge straightness
If it drifts
Cloths short on width, or a closed edge cutting into the wiping face

What you can specify Finished slit width, and how much head waste is excluded.

All 22 stages in one table

Slitting head running along the dyed roll.
Slitting head running along the dyed roll.
Cut line close up: this is the edge that gets closed two stages later.
Cut line close up: this is the edge that gets closed two stages later.
Slit strips running on, ready for the first overlock.
Slit strips running on, ready for the first overlock.

Stage 15 of 22

First overlock on the strip#

First overlock — on the continuous strip

The first overlock is a stitched edge closed along the continuous strip before individual pieces are separated.

The first overlock runs on the continuous strip, not on each piece. Both edges of the strip are closed while it is still one long length, so by the time pieces are separated every piece already has a finished edge.

Running it this way is what makes the edge consistent: stitch density and seam allowance stay the same for the whole run instead of drifting piece by piece. It is also faster, because the operators are handling one continuous length rather than hundreds of loose cloths.

What we control, and what goes wrong

The first overlock is the economical edge route. It uses thread rather than melting the fibre, so it is cheaper per piece than ultrasonic sealing, and it is the standard finish for volume programmes.

Equipment
Overlock (locking stitch) line
We control
Stitch density, seam allowance, thread tension, trim width, edge straightness
If it drifts
A wavy or puckered edge that curls after the first wash

What you can specify Stitch density in stitches per inch, and the seam allowance on the strip.

All 22 stages in one table

Strip running through the overlock line, edge being closed.
Strip running through the overlock line, edge being closed.
Overlock head and control panel: stitch density is set here.
Overlock head and control panel: stitch density is set here.
Hall view — several overlock positions running the same strip width.
Hall view — several overlock positions running the same strip width.

Stage 16 of 22

Automatic overlock to finished piece#

Automatic overlock — finished piece

Automatic overlock is the station that cuts the strip to length and closes the end edges.

After the first overlock the strip is cut to piece length and the end edges are closed on automatic stations. The result is a cloth with a stitched border on all four sides and no raw edge anywhere.

Automatic stations hold the stitch count per inch steady across a run. That is something a sample cannot prove and a bulk order depends on: the same setting produces the same seam on the thousandth piece as on the first.

What we control, and what goes wrong

Equipment
Automatic overlock stations
We control
Stitch count per inch, piece size, corner finish, thread specification
If it drifts
Seam failure on the item that gets wrung hardest — reported as “the stitching came apart”

What you can specify Stitch count per inch, corner finish and piece-size tolerance.

All 22 stages in one table

Strip running into the automatic station for the end edges.
Strip running into the automatic station for the end edges.
Finished overlocked pieces, stacked and counted.
Finished overlocked pieces, stacked and counted.

Stage 17 of 22

Manual overlock for custom shapes#

Manual overlock — irregular and customer-specific shapes

Manual overlock is hand-guided edge closing for custom or irregular outlines.

Not every item is a rectangle. Shaped wipes, contoured mitts and customer-specific outlines cannot run through an automatic overlock, so they are closed at manual stations where the operator follows the approved outline.

This is the route where the sample matters most: the outline that was approved becomes the reference, and every piece is checked against it. It costs more per piece than the automatic route, and it is the only way to close an edge that does not run straight.

What we control, and what goes wrong

We control
Operator, stitch density, outline conformity to the approved sample
If it drifts
Outline drift between the approved sample and bulk, and inconsistent stitch density between pieces

What you can specify The approved outline sample, and who signs it off.

All 22 stages in one table

Manual overlock position, operator following a shaped outline.
Manual overlock position, operator following a shaped outline.
Shaped pieces bundled by order before packing.
Shaped pieces bundled by order before packing.
Manual station in the converting hall.
Manual station in the converting hall.

Stage 18 of 22

Template sewing#

Template sewing machine — shaped seams

Template sewing is machine sewing along a path held by a jig, so a shaped seam repeats identically.

The template machine is what makes repeated shapes identical. The jig holds the piece and guides the seam, so a curved pocket or a multi-line quilt is sewn to the same path on every piece rather than by eye.

For a private-label programme the jig is also the thing that gets approved. Change the jig and the finished item changes, which is why the jig geometry belongs in the specification alongside the cloth.

What we control, and what goes wrong

Equipment
Template sewing machines with jigs
We control
Jig geometry, stitch density, seam allowance, thread
If it drifts
Shapes that differ between the approved sample and bulk, or seams that wander on a curve

What you can specify Jig geometry and stitch density - the jig is the specification.

All 22 stages in one table

Template machine: the jig holds the shaped piece while the seam is sewn.
Template machine: the jig holds the shaped piece while the seam is sewn.

Stage 19 of 22

Ultrasonic sealing and hot cutting#

Ultrasonic sealing — hot cut, hot overlock, wave or straight edge

Ultrasonic sealing is a cutting-and-fusing process in which the thermoplastic edge melts into a sealed bead.

This is the edge route for buyers whose price allows it. Instead of stitching, the thermoplastic fibre is melted at the cut line, so the edge closes itself: no thread to pull, no yarn end to shed, and a finished cloth that stays clean at the border.

The same line produces several profiles — hot cut, hot overlock, hot locking stitch, straight edge and wave edge — so the edge type has to be stated on the order. It cannot be inferred from a product photo, because the same photograph can be produced three different ways.

What we control, and what goes wrong

Ultrasonic is chosen where lint and edge quality matter more than unit cost: glass cloths, screen cloths and retail programmes where the edge is visible in the pack.

Equipment
Ultrasonic sealing line; hot cutter
We control
Seal width, line speed, bead quality, edge profile (straight, wave, hot overlock)
If it drifts
A stiffened edge, or a seal that cracks after washing

What you can specify Edge profile (straight, wave or hot overlock) and seal width.

All 22 stages in one table

Ultrasonic line with the weld heads raised over the conveyor.
Ultrasonic line with the weld heads raised over the conveyor.
Cloth passing under the heads; the edge is fused in one pass.
Cloth passing under the heads; the edge is fused in one pass.
Heat-sealed edge detail on finished cloth.
Heat-sealed edge detail on finished cloth.

Stage 20 of 22

Perforating and tear-off rolls#

Perforating — tear-off format

Perforating is the partial cutting of a sheet at intervals, so a roll holds together until a piece is torn away.

In the tear-off format the cloth is not fully cut: it is perforated, so the roll holds together until the customer pulls a sheet away. Slitting, perforating and packing are set up as one line, because the roll has to stay under tension from the first cut to the sealed bag.

The perforation depth is the whole specification. Too shallow and the sheet tears raggedly, leaving a fringe on every wipe; too deep and the roll separates in the carton before it reaches the shelf.

What we control, and what goes wrong

Equipment
Slitting, perforating and packing line
We control
Perforation pitch and depth, roll tension, sheet count per roll
If it drifts
Ragged tears, or a roll that falls apart in the carton

What you can specify Sheets per roll, perforation pitch, and whether the roll is bagged or boxed.

All 22 stages in one table

Roll running on the perforating line.
Roll running on the perforating line.
Perforated line running under the head.
Perforated line running under the head.
Perforating head: depth is set here.
Perforating head: depth is set here.
Roll being wound and bagged at the end of the same line.
Roll being wound and bagged at the end of the same line.
Packing station on the tear-off line.
Packing station on the tear-off line.

Stage 21 of 22

Packing and export marking#

Packing — retail pack, carton, marking

Packing is the stage where count, barcode, care label and carton marking are matched to the purchase order.

The last stage turns a good cloth into a shippable order. Pack count per SKU, barcode, care label wording, carton dimensions, gross weight and export marking all have to agree with the purchase order and with the destination market's requirements.

A correct cloth in a carton with the wrong barcode is a chargeback, not a shipment. Private label also becomes real here: the artwork, the bag, the header card and the hangtag are the buyer's brand from this point on, and they were approved weeks earlier.

What we control, and what goes wrong

Equipment
Packing and bagging stations
We control
Pack count per SKU, barcode, care label wording, carton dimensions and gross weight, export marking
If it drifts
Retail chargeback, or a container that cannot be received without re-labelling

What you can specify Pack count, barcode format, care label wording, carton marking.

All 22 stages in one table

Packing hall with packed product staged by order.
Packing hall with packed product staged by order.
Packing stations: count, barcode and label checked against the order.
Packing stations: count, barcode and label checked against the order.
Cartons closed and marked for export.
Cartons closed and marked for export.

Stage 22 of 22

Finished goods store#

Finished goods — ready for shipment

The finished-goods store is the order-segregated buffer where cartons wait for inspection and loading.

Cartons are stored by order and released for pre-shipment inspection and loading. The AQL inspection is carried out here rather than at the packing line, so the sample comes from the same population that will be loaded.

The lot record from the dye vessel is still attached to the order at this point. That is what makes it possible to trace a finished carton back to the batch it was dyed in, months after the shipment.

What we control, and what goes wrong

We control
Order segregation, storage condition, AQL 2.5 pre-shipment inspection, loading supervision
If it drifts
Mixed orders in one container, and no traceable lot behind a complaint

What you can specify AQL level, inspection timing and loading supervision.

All 22 stages in one table

Finished goods store: cartons stacked by order, awaiting inspection and loading.
Finished goods store: cartons stacked by order, awaiting inspection and loading.

Process index

The same twenty-two stages, in three blocks, in one table. Each row states what goes wrong when that stage drifts, and every row links back to the stage it describes — so the table can be cited on its own.

StageWhat goes wrong if it drifts
A Yarn to greige — Texturing, warping, knitting, grading and the greige store. Nothing here is dyed.
01Draw texturingBarré — bands across the finished cloth that no dye bath can correct
02WarpingWidth variation between rolls, edge curl, and a beam that has to be cut off and rewound
03KnittingA GSM that repeats on the sample and not on bulk — the commonest source of “the second shipment feels different”
04Greige inspectionMixed widths inside one carton, and cloth cut to a size that no longer matches the printed pack
05Greige storeTwo knitting lots mixed into one dye batch, with no way back to the source
B Wet processing — The greige is joined, desized and split, dyed, dewatered, opened and set. This is where the cloth becomes microfiber.
06Batch sewingA join that pulls apart mid-batch, or a seam mark that shows as a band in the finished roll
07Desizing and scouringUneven splitting, then patchy dye uptake, then a shade complaint that appears two stages later than its cause
08Alkali weight reduction (splitting)Under-reduced: soft but not absorbent, linting, streaks on glass. Over-reduced: weak cloth, chalky hand, seam failure at sewing
09DyeingUneven penetration that looks acceptable dry and goes patchy after the customer's first wash
10Centrifugal extractionWater marks set by the stenter, and rope creases that cannot be removed afterwards
11OpeningCreases set by the stenter and impossible to remove afterwards; width short of specification
12Drying, heat-setting and batchingCloth that measures correctly in the warehouse and shrinks after the first wash
C Converting — The dyed roll comes back to this building: cut, slit, overlocked, template-sewn, sealed, perforated, packed and stored.
13Back to the converting buildingTwo dye batches mixed inside one shipment — a shade complaint on an order that tested fine
14Head cutting and slittingCloths short on width, or a closed edge cutting into the wiping face
15First overlock on the stripA wavy or puckered edge that curls after the first wash
16Automatic overlock to finished pieceSeam failure on the item that gets wrung hardest — reported as “the stitching came apart”
17Manual overlock for custom shapesOutline drift between the approved sample and bulk, and inconsistent stitch density between pieces
18Template sewingShapes that differ between the approved sample and bulk, or seams that wander on a curve
19Ultrasonic sealing and hot cuttingA stiffened edge, or a seal that cracks after washing
20Perforating and tear-off rollsRagged tears, or a roll that falls apart in the carton
21Packing and export markingRetail chargeback, or a container that cannot be received without re-labelling
22Finished goods storeMixed orders in one container, and no traceable lot behind a complaint

Six things to verify before you choose a microfiber factory

This is the checklist we would want a buyer to run on us. Each line points to the stage where the claim can be seen.

CheckWhat a real factory showsStage
Yarn is textured and split in-houseTexturing machines, and an alkali line standing beside the dye vessels01, 08
Warping and knitting run on siteCreels, beams and needle beds in operation02–03
Greige is graded before dyeingAn inspection and grading area, with lot tags that travel into the dyehouse04
Splitting is measured, not assumedA weight-loss figure per lot and the resulting filament fineness08
Dyeing and setting are both controlledOverflow machines with a stated liquor ratio, and a stenter where overfeed is set09, 12
The edge route is stated per itemFirst overlock, automatic overlock, manual overlock, template sewing or ultrasonic15–19

What the stages cannot change

No finishing step makes a 200 GSM cloth behave like a 400 GSM one, and no edge route turns an 80/20 polymer ratio into a 90/10. Stage control protects the specification you ordered; it cannot substitute for it.

When a cloth feels soft in the hand and still wipes badly, the cause is almost always the splitting stage: the filaments were never fully opened. That defect cannot be seen, cannot be corrected downstream, and will not show up in a photograph.

On the numbers. What is fixed here is the sequence and the variables controlled at each stage. The values belong to a specific cloth, machine and dye recipe, so they are set per order and confirmed in the works before a run.

Terms used on this page

Draw texturing (DTY)
Heating, false-twisting and cooling a yarn to give it bulk and controlled elongation.
Greige
Cloth as it leaves the knitting machine — undyed, unfinished, still carrying knitting oil.
Batch sewing
Stitching two rolls end to end so the cloth runs continuously through wet processing.
Desizing
Washing out knitting oil and sizing before the alkali can wet the fibre evenly.
Alkali weight reduction / splitting
The caustic treatment that divides a composite filament into microfilaments.
Weight loss
Percentage of fibre mass removed by the alkali; the measurable result of splitting.
Rope form / open width
Twisted rope (dyeing) versus flat fabric (washing, stenter). Opening converts one to the other.
Overfeed
How much length the stenter lets relax into the frame; it changes finished GSM from the same greige.
Overlock / locking stitch
A stitched edge closing the cut line. Run first on the strip, then on the piece, or by hand for custom shapes.
Template sewing
Sewing along a jig-held path so shaped seams repeat identically piece after piece.
Ultrasonic sealing
Cutting and fusing in one pass; the edge melts into a bead, with no thread.
Perforating
Cutting through the sheet at intervals while leaving it held, for tear-off rolls.

Buyer questions about the process

What should I check before choosing a microfiber cloth factory?

Five things. Ask whether the yarn is textured and the cloth split in-house — a factory that buys split yarn is a converter, not a microfiber producer. Ask for the alkali weight-reduction line and the dye vessels together, because owning one without the other means the second is outsourced. Ask for a weight-loss figure per lot rather than a soft-feel claim. Ask which edge route is used per item: first overlock, automatic overlock, manual overlock, template sewing or ultrasonic are five different products. And ask for a video call from the floor at a time you choose.

How do I know the cloth is split microfiber and not fine-denier polyester?

Three tests, none needing a laboratory. Weight loss: split cloth loses mass in the alkali bath, ordinary polyester does not. Absorbency: a split cloth takes water into the filament bundle, so a drop spreads rather than beads. Edge behaviour: a cut split cloth sheds fine fibre, which is why the edge has to be closed. A supplier who cannot state a weight-loss figure is selling fine-denier polyester.

Why is the cloth overlocked before it is cut into pieces?

Because a continuous strip can be overlocked at a steady stitch density, while individual pieces have to be handled one at a time. The first overlock closes both edges of the strip, so when the piece is separated it already has finished edges — and the stitch density stays the same for the whole run.

What is the difference between overlock and ultrasonic sealing?

Overlock stitches the edge with thread; ultrasonic sealing melts it into a bead with no thread at all. Ultrasonic is cleaner and lint-free but costs more, so it is chosen where the price allows. Overlock is the economical route, and automatic overlock holds stitch density steadier than hand work.

Does the cloth leave the factory after dyeing?

No. It returns to the converting building, is booked into the ground-floor store by lot, and is cut, edge-closed, perforated or sewn and packed there. That return trip is the clearest sign of a factory that owns both the textile and the converting halves of the process.

Which stage causes linting and shedding complaints?

Two, usually together. Under-reduction at the splitting stage leaves filaments partly bonded so short fibre breaks away, and an edge that was cut rather than closed releases fibre at the border. Changing the edge route fixes the second; only correct reduction fixes the first.

Which stages run for your item, and the parameter each one governs, are set out in the specification sheet. Send a specification and we will quote it within one business day.